水性厚板浆印不厚怎么办?
时间:2023-07-22    点击次数:514

水性厚板浆印不厚怎么办?

1、选择浆料很重要、厚板浆有PU厚板浆,有普通厚板浆

2、网板一定要晒厚的网板,或把网板的四个角垫高起来

厚板浆调配比例

  厚板浆(透明)+0.5%PTF增稠剂(华樾)印厚些

  盖面:厚板浆(白)(80%)+厚板浆(透明)(20%)+0.5%PTF增稠剂(华樾),印3

  红色厚板:厚板浆(白)(20%)+厚板浆(透明)(80%)+A014大红(劳安)+0.5%PTF增稠剂(华樾),印3

工艺流程

1. 丝网选用80-100目厚板,用丝印硬方刀75度刮印, 以厚板浆(透明)打底2-3

2. 将厚板浆(白),厚板浆(透明),高温色浆搅拌匀印2-3

3. 24-48小时自然干燥,或150-180度焙烘1-3分钟

 

Product name

Waterborne thick plate pulp (glossy)

Packing

25KG/drum for white, 20KG/drum for clear

Storage

6 months in cool place

Application

Suitable for cotton, polyester etc

Features

1. High elasticity

2. High fastness

3. SGS detecting passed, no PVC, no heavy metal, no NPEOs

Mix proportion

1 Waterborne thick plate pulpClear+0.5% PTF ThickenerHY Chemical  printing thickness

2 cover: Waterborne thick plate pulpWhite (80%) + Waterborne thick plate pulpClear (20%) + 0.5% PTF ThickenerHY Chemical, printed 3 times

3 red: Waterborne thick plate pulpWhite (20%) + Waterborne thick plate pulpClear (80%) + Pigment Red A014(Laoan Chemical)+ 0.5% PTF ThickenerHY Chemical, printed 3 times

Printing process

1. Printing with Waterborne thick plate pulpClear for 2-3 times

2. Mixing with Waterborne thick plate pulpWhite, Waterborne thick plate pulpClear, pigment and stirring them evenly.

3. Printing again for 3-4 times (3-4 scrapes per time).

4. Drying it in room temperature, or baking for 1-3 minutes under 150-180

5. Finish.